MIL-PRF-44103D
(Applications for copies of referenced documents should be addressed to the American
Society for Testing and Materials, 100 Barr Harbor Drive, West Conshohocken, PA 19426-
2959.)
AMERICAN ASSOCIATION OF TEXTILE CHEMISTS AND COLORISTS (AATCC)
(Applications for copies of referenced documents should be addressed to the American
Association of Textile Chemists and Colorists, P.O. Box 12215, Research Triangle Park, NC
27709-2215.)
TECHNICAL ASSOCIATION OF THE PULP AND PAPER INDUSTRY (TAPPI)
(Applications for copies of referenced documents should be addressed to TAPPI Press,
Technology Park/Atlanta, P.O. Box 105113, Atlanta, GA 30348-5113.)
2.4 Order of precedence. In the event of a conflict between the text of this document and the
references cited herein, the text of this document takes precedence. Nothing in this document,
however, supersedes applicable laws and regulations unless a specific exemption has been
obtained.
3. REQUIREMENTS
3.1 First article. When specified (see 6.2), a sample shall be subjected to first article
inspection.
3.2 Standard sample. The finished cloth shall match the standard sample for shade and
appearance and shall be equal to or better than the standard sample for colorfastness (see 6.3).
3.3 Performance requirements. The cloth shall conform to the requirements specified in Table
I and 3.4 through 3.8.
TABLE I. Requirements
Requirements
Classes 1 & 2
Classes 3 & 4
Characteristic
Min
Max
Min
Max
2 (max)
Weight Oz/yd
--
13.5
--
15
Breaking Strength, lbs.
Warp
320
--
320
--
Filling
250
--
250
--
Tearing Strength, lbs.
Warp
11
--
11
--
Filling
7
--
7
--
Gloss (face side only) %
60° specular gloss
--
2.0
--
--
85° specular gloss
--
2.0
--
--
Adhesion of coating, lbs/2 inch width 1/:
Face and back sides
6.0
--
10.0
--
Colorfastness to:
--
Fair 2/
--
Accelerated Weathering
Fair 2/
1.5 2/
--
1.5 2/
--
Crocking, scale rating
3
For Parts Inquires call Parts Hangar, Inc (727) 493-0744